Any suggestions for reducing UV clear. I'm going to shoot test panels this weekend and would consider reducing the clear a bit to improve flow out (novice painter). Can you guys recommend that practice?

Shooting with Tekna Copper 1.3 fluid tip, 23 psi at gun, >100 psi at the wall, over solid white PPG DBU. I have slow reducer for our hot 90+ degree Sacramento weather.

thanks for the tips. Greatly enjoy the forum and the SPI products and service.

pat
 
I would test first with no reducer.
If needed start with about 2oz per mix quart and if more in needed go to 4oz.
also from people I talk to with that gun 23 sounds like it might be about 5 lbs low, never used one so only going by feedback.

Also so do keep in mind, at those temps 10% or under with that reducer will slow the clear down, over 10-15% it will start drying faster.
 