From Canada to everywhere in the country, since last week from problems to what to do, seems to be the theme.
Starting with base coat, yes it will seem like it is drying faster but the outside skims over and it causes the solvents to come out slower.
EXTEND flash times at 106 yesterday I was giving each coat of base an hour.
Four hours later I shot first coat of clear.
I waited 30 minutes exactly between all four coats of clear but I was getting nervous, that I was not waiting long enough but it worked out.
Do not rush or paint like it is 70 or you will get solvent pop, die back or worse, as one call today, first day in sun his base bubbled and let loose.
He said it was drying great and was giving it 5-10 minutes between coats at 101 degrees and using DT870 (medium) Not good.
Starting with base coat, yes it will seem like it is drying faster but the outside skims over and it causes the solvents to come out slower.
EXTEND flash times at 106 yesterday I was giving each coat of base an hour.
Four hours later I shot first coat of clear.
I waited 30 minutes exactly between all four coats of clear but I was getting nervous, that I was not waiting long enough but it worked out.
Do not rush or paint like it is 70 or you will get solvent pop, die back or worse, as one call today, first day in sun his base bubbled and let loose.
He said it was drying great and was giving it 5-10 minutes between coats at 101 degrees and using DT870 (medium) Not good.